304 vs 316 Stainless Steel: Choosing by Chloride Exposure
The 304 vs 316 question is really a chloride question. Both are 18% chromium austenitic grades; the difference is 316 carries 2–3% molybdenum, which raises pitting resistance in chloride environments. Choosing by anything else — looks, availability, habit — leads to most stainless failures in service.
Where 304 is the right call
304 handles atmospheric exposure, fresh water, food contact, most organic chemicals and mild industrial environments. For indoor structures, architectural panels, kitchen equipment and tanks holding non-saline liquids, 304 gives no practical advantage to 316 and costs less.
Where 316 is required
Once chlorides enter the picture, 316 becomes the default: coastal and marine atmospheres, de-icing salt splash zones, brackish water, and process streams above roughly 200 ppm chloride. Pitting on 304 in these conditions starts as small rust-colored dots and progresses quickly because the pit itself concentrates chloride. 316 pushes the threshold up, but it is not immune — frequent salt-wash down still matters.
Temperature raises the stakes
Chloride stress corrosion cracking above about 50 °C is the second failure mode, and molybdenum does not fix it. Hot chloride service — heat exchanger shells, hot brine lines — needs a duplex grade such as 2205 or a stabilized grade, not simply "316 instead of 304".
What to state on the order
Specify grade plus finish (2B, No.1, brushed), the applicable standard (ASTM A240 or EN 10088-2), and certificates to EN 10204 3.1. If the service environment is aggressive, ask for the mill's composition report and check that molybdenum is actually within 316's range — mislabeled 304 sold as 316 is a real and expensive problem.
Short version: dry or fresh water, order 304; chlorides present, order 316; hot chlorides, move to duplex. The previous articles in this series cover 321 stabilization and 2205 duplex selection for those cases.